High-speed X-rays have caught a pore forming inside molten titanium alloy, revealing a defect hidden from surface cameras. In a study published on June 15, 2017, researchers at Argonne National Laboratory, Carnegie Mellon University and Missouri University of Science and Technology recorded laser heating at 50,000 frames a second. For manufacturers investigating flawed parts, the experiment shows how similar-looking surfaces can conceal different interiors. It is not a production-line inspection system. [S2]

The team tested miniature beds of Ti-6Al-4V titanium-alloy powder at Argonne’s Advanced Photon Source. At 340 watts, a one-millisecond laser pulse left a dome-shaped surface without noticeable structural defects. A 520-watt pulse of the same duration also left a dome, but with a pore roughly 150 micrometers across deep in the metal base. The laser spot was about 220 micrometers wide. These were stationary heating tests, with no laser scanning—not a comparison of complete printed parts. [S2]

The images showed how the void survived. Strong heating drove metal vapor out of the pool and pushed liquid aside, creating a deep cavity. When the laser switched off, liquid flowed back toward the center. In the higher-power case, the bottom did not fill quickly enough, leaving a pore that could not reach the surface before the advancing solid metal trapped it. That gives process engineers a specific sequence to investigate: what happens when the beam stops and the melt cools. [S2]

Seeing the boundary of the molten pool took more than a fast camera. The authors’ supplementary methods describe dividing each image by the image taken before heating, then analyzing brightness along horizontal lines to locate the cavity and liquid–solid boundaries. They connected and smoothed those points to estimate the pool’s outline and area. The paper notes that the small density difference between liquid and solid titanium alloy makes the outer boundary difficult to identify. The measurement therefore includes an image-processing method, not simply a visible line traced from a photograph. [S2][S3]

The particle measurements required judgment too. The supplement says software located candidate particles and tracked them through enhanced images, with people checking both the initial locations and the resulting tracks. The main paper adds that particle velocities are projections onto a two-dimensional image plane: motion along the X-ray beam is missing. A manufacturer evaluating these data would need the tracking procedure and viewing geometry, not just a maximum speed copied from a chart. [S2][S3]

The authors propose using these measurements to improve models and guide process settings, while acknowledging that precise control of a printed metal’s internal structure and properties remains difficult. The study supplies no factory rejection-rate reduction or cost-saving figure. Its 340- and 520-watt observations belong to the stated alloy, beam and miniature test setup; they are not general-purpose safe and unsafe power settings for a printer. [S2]

Source documents

  1. Real-time monitoring of laser powder bed fusion process using high-speed X-ray imaging and diffractionhttps://www.nature.com/articles/s41598-017-03761-2
  2. Supplementary Material for Real-time monitoring of laser powder bed fusion process using high-speed X-ray imaging and diffractionhttps://media.springernature.com/original/springer-static/esm/art%3A10.1038%2Fs41598-017-03761-2/MediaObjects/41598_2017_3761_MOESM10_ESM.pdf